White oak is the slowest and most check-prone of the common Missouri hardwoods. Red oak and hickory come next. Walnut, cherry and hard maple dry at a moderate pace, and ash and soft maple give up water fastest. Each one also has its own way of going wrong: white oak checks and honeycombs, walnut needs care with its pale sapwood, maple stains if it dries too slowly, and ash draws powderpost beetles.
The table puts the numbers side by side. The species pages explain what to do about them.
The common Missouri hardwoods, compared
| Species | Green moisture content, heartwood / sapwood | Safe drying rate, 4/4 (% per day) | Kiln days, 4/4 from air-dried / green | Watch for |
|---|---|---|---|---|
| White oak | 64% / 78% | 2.5 | 5 / 23 | Surface checks, honeycomb |
| Red oak (northern) | 80% / 69% | 3.8 | 5 / 21 | Surface checks, honeycomb |
| Hickory | Varies by species | Not listed | 4 / 10 | Sapwood stain, powderpost beetles |
| Black walnut | 90% / 73% | 8.2 | 5 / 11 | End checks; pale sapwood |
| Cherry | 58% heartwood | 5.8 | 5 / 10 | Few; honeycomb in wetwood (not common) |
| Hard (sugar) maple | 65% / 72% | 6.5 | 5 / 11 | Sticker stain, gray sapwood stain |
| Soft maple (silver) | 58% / 97% | 13.8 (sapwood) | 4 / 7 | Sapwood stain if dried slowly |
| White ash | 46% / 44% | 10.4 | 4 / 10 | Gray-brown sapwood stain, powderpost beetles |
Sources: green moisture content from the Wood Handbook, ch. 4, Table 4–1; safe drying rates and minimum kiln days (to 6 percent in conventional kilns) from FPL-GTR-118, Tables 8.6 and 7.25.
Two things in that table surprise people. First, wetter isn't slower: walnut heartwood starts out far wetter than white oak heartwood but dries much faster, because white oak's pores are plugged. Second, the gap between "from air-dried" and "from green" is biggest for the oaks. Air-drying oak before the kiln saves the most time.
Easy, moderate and hard to dry
FPL's drying manual sorts hardwoods into three groups for choosing a drying method. Oak and beech are its examples of hard-to-dry species; hickory and hard maple are moderately hard; ash, basswood, yellow-poplar and soft maple are easy. The hard-to-dry group gains the most from a careful start, under a roof or in a predryer, before the kiln. The easy group gains the most from speed, because its risk is stain, not cracking.
White oak
The slowest common hardwood, held to the gentlest kiln schedules. Its heartwood pores are blocked by growths called tyloses, so water leaves slowly, and the surface checks if it's pushed. Air-dry it under a roof and give it extra time at every thickness. Drying white oak
Black walnut
Moderate and fairly forgiving, but thick walnut can end-check and honeycomb, and its pale sapwood contrasts with the dark heartwood. Steaming before drying is the usual way to even out the color. Drying black walnut
Maple
Hard maple dries at a moderate rate; soft maple is fast. Both are prized for pale wood, and both stain if they dry too slowly at warm temperatures: gray sapwood stain, and sticker stain that shows only after planing. Speed and airflow are the cure. Drying maple
Ash
Low green moisture content and a fast safe drying rate make ash one of the easiest Missouri hardwoods to dry. The catches are gray-brown sapwood stain if it sits wet, and powderpost beetles, which favor large-pored hardwoods like ash. Drying ash
Mixing species in one load
Kilns run one schedule for the whole chamber, so a load is only as fast as its slowest board. FPL's manual advises drying one species at a time, or a few with similar drying characteristics. White oak can't share a schedule with ash or soft maple without either slowing them down or risking checks in the oak. That's why kiln loads are grouped by species and thickness.
For general timelines, see drying times. For the target number at the end, see moisture content.
Join the Waitlist
Tell us which species you have and how thick. A waitlist heavy in white oak needs a different kiln plan from one full of ash.