COLUMBIA
KILN DRYING
Join the Waitlist

Status · November 15, 2026: planned, not installed. We are not accepting wood.

Drying Ash Lumber and Slabs

Ash is one of the easiest hardwoods to dry. It starts out with relatively little water and tolerates fast drying, and FPL flags surface checking only in 6/4 and thicker ash. Inch-thick ash stacked in spring reaches about 20 percent moisture content in something like 45 to 80 days across much of Missouri, and FPL's kiln minimums are just 4 days from air-dried and 10 from green. Manage two risks: stain in the sapwood if the wood stays wet too long, and insects, since lyctid powderpost beetles like ash. A kiln's heat deals with the insects.

If your ash came from a tree killed by emerald ash borer, it dries the same way as any other ash. The bug questions just matter more.

How fast it gives up water

White ash is unusually dry for a green hardwood. Table 4–1 of the Wood Handbook lists it at about 46 percent moisture content in the heartwood and 44 in the sapwood, with green ash sapwood at about 58. Compare black walnut heartwood at 90 percent. Less water to remove means a shorter trip.

It also tolerates speed. White ash can safely lose 10.4 points of moisture a day as 4/4 and 4.1 as 8/4, roughly four times white oak's limit, according to Table 8.6 of the USDA Forest Products Laboratory's drying manual. FPL's manual names ash among its examples of easy-to-dry species, alongside basswood, yellow-poplar and soft maple.

Air-drying timeline by thickness

Stock What to expect
4/4 45–80 days; ends near 20%
8/4 180–230 days; ends in the mid-20s
Thicker No FPL figure; plan on 2½ to 3+ years to air-dry fully

Ranges are FPL's for its Central zone, which takes in much of Missouri (Table 4.2); spring and early-summer stacking gets the short end. The thick-stock line is the usual year-per-inch estimate.

Because ash dries readily, the air-drying risk is less about checking and more about what happens while it sits: stain in the sapwood and insects moving in. Stack it soon after sawing, off the ground, on dry stickers, under a roof. Our air drying guide has the details.

Kiln schedule notes

FPL's schedules for white and green ash begin at 130°F (4/4) or 120°F (8/4) while the wood is wet, and carry the comment "normal color; some darkening."

Starting point Minimum kiln days, 4/4 ash
Air-dried, about 20% 4
Green 10

White and green ash in a conventional kiln, to about 6 percent (FPL-GTR-118, Table 7.25). FPL says to allow at least a quarter more for real loads; 8/4 takes 2.5 times as long.

Kiln drying also takes care of insects: a normal steam or dehumidification schedule gets ash hot enough, for long enough, to kill beetles and their eggs. Our lumber sterilization page has the temperatures and heating times.

Emerald ash borer is a special case. It takes more heat than ordinary pests: the Wood Handbook cites a USDA schedule calling for ash wood's core to hit 140°F and stay there an hour or more (ch. 20). A conventional or dehumidification kiln on a normal ash schedule runs above 140°F near the end, but if you need treatment documented for moving ash wood, that's a separate question to ask.

Typical defects

FPL's defect table names two for white ash:

  • Gray-brown sapwood stain, including stain under the stickers. FPL ties it to trees from wet sites, drying too slowly and poor airflow.
  • Surface checks in 6/4 and thicker stock. Ash is forgiving in 4/4, less so in thick planks and slabs.

Powderpost beetles. Not a drying defect, but the most common complaint with ash. In Oklahoma State University Extension's list of the woods the southern lyctus beetle infests most, ash comes first, ahead of hickory and oak. OSU also names farm-sawed lumber as a frequent source of infestations. Look for pinholes and fine powder, heat the wood through, and keep it dry and finished afterward. Our sterilization page covers identification and treatment.

Target moisture content

Dry ash for furniture, flooring or trim to 6 to 8 percent. That sits inside the 6-to-10 indoor range in MU Extension's G5507. In width, flat-sawn white ash moves about like walnut: its Wood Handbook coefficient is also 0.00274, which works out to roughly 0.11 inch on an 8-inch board dried from 12 to 7 percent.

For tool handles and other bent or turned work, ask before drying; FPL notes that some specialty products are dried to a higher moisture content than furniture lumber.

See drying by species for the other woods, or moisture content targets for the meter work.

Join the Waitlist

Sawing ash from a tree that came down? Tell us how much, how thick, and whether you've seen any small holes or powder.

Join the Waitlist

HELP SHAPE THE PLANNED KILN

What wood would
you bring?

Share your species, thickness and board feet. We’ll email you before the kiln opens.

Join the Waitlist