Air dry lumber on a level foundation a foot or more off the ground, with dry stickers lined up in straight columns over each support, a roof that overhangs the stack by about 2 feet with air space beneath it, weight on top, and sealed ends. Point the stack so the prevailing wind blows across the boards. In Missouri, that gets most hardwood down to about 20 percent moisture content in one warm season for 1-inch boards, and around 12 to 14 percent eventually, which is as dry as outdoor air allows.
Every number on this page comes from MU Extension's guide Air-Drying Hardwood Lumber (G5550) unless noted. It's the best short guide for Missouri conditions, and worth printing.
Site and foundation
Pick the spot. MU recommends a level site with good drainage and exposure to the prevailing winds. Orient the stack so those winds blow across the boards, not along them. Black polyethylene on the ground under and around the stack helps keep ground moisture from rising into the bottom layers.
Clean it up. The USDA Forest Products Laboratory's drying manual points out that piles of slabs, sawdust, bark, old lumber and broken stickers are breeding grounds for insects, and that clearing them removes most insect problems (FPL-GTR-118). Don't build a new stack next to last year's scrap pile.
Build the foundation. MU wants the bottom layer of boards a foot or more above the ground, on supports spaced 24 inches apart at most. They need to be level and in one flat plane, because every board in the stack will take the shape of the foundation as it dries. Concrete blocks with treated timbers across them work well; check them with a long straightedge.
Size the stack. MU suggests going no higher than you can stack comfortably and safely, usually head-high. FPL notes that in air drying, narrower piles dry faster.
Sticker spacing and alignment
Stickers are the thin spacer strips between layers. They're the difference between a stack that dries and a pile that rots.
Size and wood. MU gives stickers as commonly 1 inch thick by 1½ inches wide, as long as the stack is wide. FPL's manual adds that stickers should be uniform in thickness, straight-grained and dry; it recommends 8 to 10 percent moisture content for stickers to prevent sticker stain. Wet stickers make dark stripes across light woods like maple and ash.
Spacing. For upper-grade 4/4 to 6/4, FPL suggests 12 to 18 inches; for anything thicker than 6/4, 24 inches usually does. Add a sticker within 12 inches of each end of the stack so board ends don't hang free.
Alignment. This is where most home stacks fail. MU says to place stickers directly over the foundation crossbeams; FPL adds that each sticker has to sit exactly over the one beneath it, in an unbroken column to the foundation, and that being off by an inch or two can make warp much worse. Lay a string line or mark the sticker positions on the end boards before you start.
Gaps between boards. MU recommends leaving 1 to 2 inches between boards in each layer, so air can move up through the stack as well as across it.
One thickness per layer. Keep each layer to boards of the same thickness. A thinner board in a thick layer isn't held flat by the stickers above it.
Our guide to stickers: thickness, spacing and stain goes deeper.
Roof and weight
Roof. MU's specification: the roof overhangs the stack by 24 inches on the front, back and both sides, and sits 6 inches above the top layer so air can move under it. Cover the top, not the sides; the sides have to breathe. Corrugated metal or plywood on a few spacer boards works.
The roof pays for itself. FPL cites a study in which pile roofs saved enough in degrade and drying time on 4/4 red oak to pay for themselves in five uses, and research in which roofed piles came out more than 5 percent drier than unroofed ones through rainy autumn and winter seasons.
Weight. MU notes that warp can be minimized by stacking properly and adding weight to the top of the stack. Concrete blocks or scrap steel spread over the top layer, sitting on the stickers, keep the upper boards from cupping and twisting as they dry.
End sealing
End grain loses water several times faster than faces and edges, MU says, so the ends shrink first and split. Coating them with a commercial wax emulsion sealer reduces that checking.
The difference is dramatic. FPL's manual reports a summer test on red oak logs in Wisconsin: after 12 weeks, uncoated ends had split about 6 inches deep, while coated ends had no splits at all. Boards behave the same way on a smaller scale.
- Seal the same day the wood is sawn, or as soon as you can.
- Coat the whole end grain heavily, including any cracks already there.
- Recoat after any crosscut.
MU notes that end coating slows drying and is worth it for higher-quality lumber. For furniture-grade walnut, oak, cherry and maple, and for any slab, it is.
How dry it will get outdoors
Not dry enough for indoor furniture. MU's air-drying guide says correct outdoor exposure can bring lumber to 14 to 19 percent moisture content, and MU's drying overview gives 12 to 14 percent as typical for Missouri lumber dried in the open air (G5507). The Wood Handbook's figures for St. Louis show why it stops there: outdoor air holds wood between about 12.3 and 14.3 percent through the year (Wood Handbook, ch. 13).
That's still useful:
- Below 20 percent, MU says, wood is no longer susceptible to decay or sap stain.
- 15 to 20 percent is adequate for unheated buildings such as garages and barns.
- For furniture and other indoor work, MU says further drying to 6 to 8 percent in a kiln is required.
How long it takes depends on thickness and when you stack. MU notes that 2-inch lumber can take two to four times as long as 1-inch, and that in its example chart, 8/4 lumber stacked on August 1 needs almost 320 days to reach 20 percent. FPL's model for Columbia, Missouri, puts 1-inch red oak at about 7 weeks if stacked in late June and about 5 months if stacked in late October. Our drying times page has the full tables.
When it's ready for a kiln
Lumber is ready for the kiln at about 20 percent moisture content for most hardwoods, and 25 percent for oak and hickory. Those are the "air-dried" starting points in FPL's kiln-time tables. Air drying to that point first cuts kiln time sharply: FPL's minimum for 4/4 white oak is 5 days from air-dried against 23 from green. The Wood Handbook adds that air drying to 20 to 25 percent before kiln drying saves energy, because kilns are the most energy-hungry step in making lumber.
To check, use a pin meter with the pins driven well into the board, not just the surface, on several boards from the middle of the stack, where drying is slowest. Our moisture content guide explains how to read thick stock.
If your wood has reached 20 to 25 percent and you're waiting on a kiln, leave it stacked and covered. It will keep inching down toward outdoor equilibrium, and every point it loses is time it won't need in the kiln.
Join the Waitlist