Use stickers about ¾ inch thick and 1¼ to 1½ inches wide, all the same thickness, made from dry, straight-grained wood. Space them 12 to 18 inches apart for 4/4 to 6/4 lumber you want flat, and up to 24 inches for thicker stock. Stack them in perfect vertical columns over the foundation supports. And keep them dry: wet stickers and slow drying are behind the dark stripes called sticker stain.
That's the USDA Forest Products Laboratory's guidance in brief. Here's the reasoning behind each number.
Thickness
FPL's drying manual says the typical sticker thickness for air drying is ¾ inch, with ⅞ and 1 inch occasionally used. For kiln drying it's usually ¾ inch, with anything from 9/16 to ⅞ inch in use (FPL-GTR-118). MU Extension's air-drying guide describes 1 by 1½ inches as common (G5550). Either works for a home stack.
What matters more is that every sticker in the stack is the same thickness. FPL says nonuniform thickness increases warp, because a thin sticker leaves a board unsupported and a thick one creates a high spot.
Thicker stickers do move more air, but in a kiln they cost space. FPL's rule of thumb: each ⅛ inch of added sticker thickness reduces kiln capacity by 7 percent.
Width and strength
FPL gives 1¼ to 1½ inches as the usual width for hardwood drying. Width doesn't affect drying much, but two things go wrong at the extremes:
- Too wide may encourage staining under the sticker.
- Too close to square gets stickers laid on edge by accident, which changes their thickness and causes warp.
FPL also notes that a sticker's strength depends on its width times its thickness squared. A sticker twice as wide is about twice as strong; one twice as thick is about four times as strong. Thin stickers in a tall stack of heavy slabs can crush or break.
Wood and condition
Dry. FPL recommends stickers at 8 to 10 percent moisture content, checked with a meter. A wet sticker keeps the board wet where they touch, exactly the condition that starts stain.
Straight-grained and uniform. Stickers that bow or twist pass the shape along.
Strong. FPL notes that the heartwood of a durable species is often suggested, and that a strong species like oak is commonly used because stickers are an investment that gets reused.
Grooved, if you can. Grooved stickers, with ridges that cut the contact area, have been used effectively to prevent stain, FPL says. It also reports that stickers made from recycled plastic and wood greatly reduce the risk of stain.
Long enough. At least as long as the stack is wide; FPL notes they're often made 1 to 2 inches longer, which helps line them up and lets you check alignment by eye from the side.
Spacing
From FPL's manual:
| Stock | Sticker spacing |
|---|---|
| Upper-grade 4/4 to 6/4 hardwood, where flatness matters | 12 to 18 inches |
| Lower-grade 4/4 to 6/4, more prone to warp | About 12 inches |
| Hardwood thicker than 6/4 | 24 inches usually acceptable |
| Warp-prone species | About 12 inches |
| Random-length stacks | An extra sticker within 12 inches of each end |
Closer spacing costs a few more stickers and saves a lot of warp. For valuable 4/4 boards, err toward 12 inches.
Alignment
This is the step most home stacks get wrong, and FPL is blunt about it: stickers must line up directly above and below each other, all the way down to the foundation, and even 1 or 2 inches of misalignment can greatly increase warp. Where flatness matters, FPL also says to put a bolster, the heavier crosspiece under the stack, under every column of stickers so each column is supported to the ground.
Two practical tricks: mark sticker positions on a long board laid on each side of the stack and work to the marks, and stand back after every few layers and sight down the columns.
Why stickers stain
Sticker stain, which graders also call sticker shadow, is a band of discolored wood across a board exactly where a sticker sat. It's usually darker, sometimes lighter, and often invisible until the board is planed. FPL says fungi are seldom involved and the stained wood is nearly always as strong as the rest.
The cause. FPL explains that sticker stain starts when lumber dries slowly, under about 5 percent moisture loss per day, at warm temperatures between 50°F and 130°F, while it's still above 40 percent moisture content. That sets off a chemical reaction in the wood under the stickers that shows up much later. High kiln temperatures near the end of drying make it more visible. FPL is clear that the stickers themselves don't cause the stain, though some sticker woods may make it slightly worse.
Who gets it. Pale woods, where it shows: maple, ash and the other light-colored hardwoods. FPL cites research finding it almost unavoidable in lumber sawn from old, stored logs.
How to prevent it. FPL's list for lumber at risk includes:
- Saw fresh logs, and in warm weather stack the lumber within 12 hours of sawing.
- Use dry stickers, 8 to 10 percent moisture content, about 1¼ inches wide by ¾ or ⅞ inch thick.
- Use grooved stickers.
- Keep rain off freshly stacked lumber.
- After a few days of drying, restack with dry stickers placed a few inches from the original spots.
- Get the lumber drying fast: good airflow, and into a kiln or fan shed early.