Drying Black Walnut Lumber and Slabs

Black walnut is one of the more forgiving hardwoods to dry. Stacked in spring in much of Missouri, inch-thick walnut needs something like 45 to 80 days to come down to about 20 percent moisture content, and 2-inch walnut 180 to 230 days to reach the mid-20s. In a conventional kiln, FPL's minimums are 5 days for air-dried 4/4 and 11 days from green. The things to watch are the ends, which check fast, thick stock, which can honeycomb, and the pale sapwood, which some woodworkers darken by steaming before drying.

When walnut is sawn into wide, thick slabs, that's where most of the trouble starts.

How fast it gives up water

Walnut starts out wet and dries steadily. Its heartwood averages about 90 percent moisture content when green and its sapwood about 73, per the green-wood table in chapter 4 of the Wood Handbook. Unusually, the heartwood is the wetter of the two, so a slab with a lot of dark wood carries a lot of water.

Despite that, walnut moves water out much more readily than oak. The USDA Forest Products Laboratory sets its safe drying rate at 8.2 percentage points per day for 4/4 and 3.3 for 8/4, more than three times what white oak can take (FPL-GTR-118, Table 8.6). Its specific gravity, 0.51, is moderate for a hardwood, and lighter woods generally dry faster.

That doesn't make it foolproof. FPL groups black walnut with the oaks and beech as woods "more likely to check or honeycomb during kiln drying" than light, easy species. Thickness is usually what tips it over.

Air-drying timeline by thickness

FPL's drying manual gives walnut the same ranges as cherry, ash and sugar maple in its Central zone, which takes in much of Missouri (FPL-GTR-118, Table 4.2):

  • 4/4: 45 to 80 days to reach about 20 percent.
  • 8/4: 180 to 230 days to reach the mid-20s.
  • 10/4 and thicker: no published figure. Plan in years: woodworkers' usual estimate of a year per inch puts 10/4 at two and a half years and 12/4 at three or more to air-dry fully.

The short end of each range assumes stacking in spring or early summer. Stack in fall and the wood sits nearly idle through winter.

Seal the ends immediately. Walnut end-checks quickly, and the checks don't always stay at the ends. Writing about walnut gunstock blanks, FPL warns that without a quality end coating, end checks can extend through the length of the piece as honeycomb. For thick slabs and turning blanks, coat the ends heavily the day they're cut, and recoat any fresh cut. MU Extension recommends a commercial wax emulsion sealer (G5550).

Our slab drying page covers stacking wide walnut slabs.

Kiln schedule and steaming notes

FPL's recommended schedule for 4/4 walnut starts at 120°F while the wood is wet; 8/4 starts gentler, at 110°F. The Wood Handbook prints a complete moisture-content schedule for 1-inch black walnut dried to 7 percent: it holds 120°F with humid air until the wood drops below 30 percent, then climbs in steps to 180°F once the wood is below 15 percent, and ends with equalizing and conditioning at 180°F (Wood Handbook, ch. 13, Table 13–3).

For time in the kiln, FPL's Table 7.25 gives 4/4 walnut a minimum of 5 days from air-dried stock and 11 from green, to about 6 percent. Actual runs take at least a quarter longer than the table, and 8/4 takes two and a half times as long as 4/4.

Steaming. Walnut sapwood is much paler than the heartwood. FPL says the most common use of presteaming is to darken black walnut sapwood and tone down that contrast, and that steaming also makes the heartwood color more uniform. FPL is also candid that little research has been done on steaming and its advice should be applied with caution. Whether to steam is a choice, not a fix: plenty of woodworkers want the sapwood contrast in a live edge piece.

FPL also reports that freezing walnut before drying sped drying and reduced losses in lab tests, though larger tests haven't always shown the same benefit.

Typical defects

FPL's defect table (Table 7.2) lists three problems for black walnut:

  • End checks, from severe drying. The main loss in walnut, and the reason to seal ends fast.
  • Iron stain, from walnut's extractives reacting with iron and water. Keep bare steel, rusty fasteners and wet steel tools off the wood.
  • Honeycomb, collapse and ring failure, associated with wetwood.

Pale sapwood isn't a drying defect, but it's what walnut buyers notice first. If you plan to use the sapwood, dry the wood steadily: the Wood Handbook notes that blue stain fungi grow in sapwood, not heartwood, and get established when wood dries too slowly at the start, a common summer problem (Wood Handbook, ch. 13). Get walnut stickered and air moving through it soon after it's sawn.

On the plus side, FPL notes that walnut's heartwood resists decay and insects, much as white oak's does.

Target moisture content

Walnut headed for furniture or cabinets should come down to 6 to 8 percent, the low end of the range MU Extension gives for wood inside Missouri homes. Once there, it's reasonably stable. Take an 8-inch flat-sawn walnut board from 12 percent down to 7: the Wood Handbook's tangential coefficient for walnut is 0.00274, so it loses 8 × 0.00274 × 5 = about 0.11 inch of width. White oak would lose about 0.15 inch.

A wide slab moves proportionally more. Size your fasteners and joinery for it, and check the core before you flatten (see moisture content targets).

For other species, see drying by species.

Join the Waitlist

Have walnut boards or slabs drying? Tell us the thickness, the widest piece and the date it came off the saw.

Join the Waitlist

HELP SHAPE THE PLANNED KILN

What wood would
you bring?

Share your species, thickness and board feet. We’ll email you before the kiln opens.

Join the Waitlist