All three come from the same cause: the outside of a board drying and shrinking before the inside. Surface checks are cracks that open early, when the dry shell is pulled tight around a wet core. Honeycomb is internal cracking late in drying, when the stresses reverse and the core is torn apart. Case hardening is the stress left behind in a board that dried without cracking, and you only see it when you rip or resaw the board and it bows or pinches the blade.

A good kiln schedule is built to prevent all three. Here's how each one forms and how to spot it.

How drying stress builds and reverses

The USDA Wood Handbook explains the sequence (ch. 13):

  1. Early in drying, the surface fibers dry first and try to shrink. The wet core hasn't started shrinking, so it holds the shell back. The shell goes into tension, the core into compression.
  2. If the shell dries too fast, it's stretched past its elastic limit and dries in a permanently stretched, or "set," condition without shrinking fully. Surface checks can open at this stage.
  3. Later, the core dries and tries to shrink, but the set shell is now too big for it. The stresses reverse: the shell goes into compression, the core into tension.
  4. If that core tension is severe enough, the core cracks internally. That's honeycomb.

The Wood Handbook adds that drying stresses are the main cause of drying defects other than stain, and that the kiln schedule is limited by them: it has to dry as fast as possible without letting the stresses exceed the wood's strength at each stage.

Surface and end checks

What they are: cracks on the faces (surface checks) or ends (end checks), opening early in drying. The Wood Handbook says surface checks occur most often on the faces of flat-sawn boards.

When they form: early. The USDA Forest Products Laboratory's drying manual ties the risk to the first third of moisture lost: green down to roughly 50 percent in red oak, roughly 45 in white oak (FPL-GTR-118). After that it's "virtually impossible" for new checks to form, except under extreme conditions, because the shrinking core is now pressing on the shell. Checks can reopen later, but they were made early.

What causes them: drying too fast, meaning humidity too low, air too fast, or both; excessive temperature contributes. For end checks, the ends simply dry far faster than the rest.

How to tell when a check formed: FPL's tell: dirt or stain inside a check means it was already open during air drying. A clean, bright check probably opened later.

How kilns prevent them: FPL's advice for check-prone woods includes keeping initial temperatures at or below 110°F, holding humidity high during the first stage, limiting air speed, and watching the daily drying rate so no sample loses moisture faster than the species' safe limit. End coating stops most end checks.

Honeycomb

What it is: internal cracks that may not show on the surface at all. The Wood Handbook says honeycomb forms in the later stages of kiln drying when the core is in tension, still at a fairly high moisture content, and the temperature is too high for too long. It may go unnoticed until the lumber is machined.

Who gets it: FPL's defect table lists honeycomb for oak, walnut, hickory, and maple heartwood, among others, often tied to severe drying of heartwood or to wetwood. MU Extension lists honeycomb among the results of extreme drying (G5507).

How to find it: crosscut a board near the middle and look at the end grain. Honeycomb shows as checks inside the cross-section that don't reach the faces. The Wood Handbook notes that speed-of-sound testing has proven effective at detecting it without cutting.

What it means: it can't be repaired. Boards with honeycomb lose the affected length.

Collapse

A cousin of honeycomb. The Wood Handbook describes collapse as flattening or crushing of wood cells. Severe collapse shows as grooves or a washboard surface; mild collapse just looks like extra thickness shrinkage. FPL's table ties it mostly to wetwood in species such as oak, walnut and maple.

Case hardening

What it is: residual drying stress in a board that's otherwise dry and sound. FPL notes the name is misleading, because the surface doesn't actually get harder; the shell is simply locked in compression around a core in tension.

What it does: FPL says it causes warp when lumber is machined, gluing problems, and pinching of the saw blade during ripping or resawing. Typical signs:

  • A board rips and the two halves spring apart or pinch together on the blade.
  • A resawn board cups or bows soon after the cut.
  • A board warps after it's planed or machined.

How to test for it: FPL's prong test. Cut a cross-section about an inch long from a dried board. Saw out the center, leaving two outer prongs joined at one end. If the board has residual stress, the prongs curve inward as the core's tension is released; with moderate to severe stress, they touch. FPL cautions that the test is most accurate after the wood has cooled and any temporary moisture differences have evened out, which can take several days after drying, and that the prongs should rest a few hours in a warm room before you judge them.

How kilns fix it: conditioning. After the load is dry and equalized, the kiln raises the humidity briefly so the shell takes on a little moisture and its compression is relieved. FPL says denser species and thicker lumber need longer conditioning: as little as 4 hours for low-density 4/4 hardwood, up to 48 hours for dense 8/4. FPL also notes that wood dried in a dehumidification kiln develops normal case hardening stresses, which must be relieved with a small boiler or water spray if the wood will be resawn, ripped or heavily machined.

Reverse case hardening: overdo the conditioning and the shell ends up in tension instead. FPL says there's no cure except heavy, equal planing of both faces.

What you can do as a woodworker

  • Don't rush air drying either. Hot, dry wind and direct sun on a stack can check oak just as a bad kiln can. Our air drying guide covers roofs and shade.
  • Seal ends on fresh-sawn stock right away.
  • Ask whether kiln-dried lumber was conditioned, especially if you plan to resaw it.
  • Prong-test a cutoff before resawing a valuable board.
  • Crosscut a sample of thick stock before committing it to a project, and look for internal checks.

See drying times for safe drying rates by species, and drying white oak for the species most prone to all of this.

Join the Waitlist

Tell us what species and thickness you're drying, and whether you plan to resaw it. Wood that will be resawn needs its stress relieved.